| Unit | ZrO2 white | ZrO2 black | Al2O3 | Si3N4 | ZTA | ||
| Composition | ZrO2 Y2O3 |
ZrO2 Y2O3 Pigment |
Al2O3 | Si3N4 Y2O3 Al2O3 |
Al2O3 ZrO2 |
||
| Mechanical properties | |||||||
|
Sintered parts Young’s modulus |
Gpa |
200 |
200 | 400 | 320 | 300 | |
| Sintered density | g/cm3 | ≥ 6.06 | 5,95 | 3,9 | 3,2 | 4,2 | |
| Bend strength | as-fired | Mpa | 600 - 800 | 400 - 600 | 400 | 600 | 500 |
| polished | 800 - 1.000 | 600 - 800 | - | - | - | ||
| Fracture toughness | MPa ·m½ | 6 - 9 | 5 - 6 | 3,5 | 8 | 7 | |
| Hardness (Vickers) | HV | 1.350 | 1.350 | 2.000 | 1.600 | 1.800 | |
| Thermal properties | |||||||
| Expansion coefficient | 10-6/K | 10 | 10 | 8 | 3,2 | 8 | |
| Conductivity | W/mK | 2 | 2 | 30 | 30 | 23 | |
| Thermal shock resistance | °C | 350 | - | 200 | - | - | |
| Max Operating temperature | °C | 400 | 400 | 1.600 | 1.200 | 1.600 | |
| Electrical properties | |||||||
| Resistance | Ω m | 108 | - | 1012 | - | - | |
| Dielectric constant | 22 | - | 10 | - | - | ||